Tuesday, 7 February 2017

Monel 400/ UNS N04400/ DIN W.Nr 2.4360 and 2.4361 Characteristic, Corrosion Resistance and Fabricating

Monel 400 Alloy Characteristic


Monel 400/UNS N04400/ DIN W. Nr 2.4360 and 2.4361 is a high strength and excellent resistance nickel copper alloy 400. Alloy 400 is widely apply in many fields, marine and chemical processing, electrical and electronic, pumps and valves, heat exchangers and feedwater heaters, deaerating heaters, etc.

Alloy 400 Corrosion Resistance:

Monel alloy 400 exhibits resistance to corrosion by many reducing media. It is also generally more resistant to attack by oxidizing media than higher copper alloys. This versatility makes alloy 400 suitable for service in a variety of environments.

Alloy 400 offers exceptional resistance to hydrofluoric acid in all concentrations up to boiling point. It is perhaps the most resistant of all commonly used engineering alloys. Alloy 400 is also resistant to many forms of sulfuric and hydrochloric acids under reducing conditions.

Fabricating for Monel 400

Monel alloy 400 is softer than many steels. The range of hot- forming temperatures is 1200℉ to 2150℉. For heavy reductions, recommended metal temperatures is 1700℉ to 2150℉. Light reductions may be taken down to 1200℉.



Sunday, 22 January 2017

Inconel 690 alloy/ UNS N06690/ WNR 2.4642 characteristic, Chemcial composition & Fabrication

Inconel 690 alloy Characteristic



Inconel 690 is a high-Chromium nickel alloy, which is a excellent resistance to fluoride containing hot nitric acid, to stress corrosion cracking caused by alkalis and media containing chloride and polythionic acids, and to many aggresstive aqueous media or in the primary and secondary loops of nuclear reactors. And good resistance to oxidation, sulphidation and metal dusting in hot gases.

Inconel 690 alloy chemical composition:

Ni: ≥58.0
Cr: 27.0-31.0
Fe: 7.0-11.0
C: ≤0.05
Si: ≤0.50
Mn: ≤0.50
S: ≤0.015
Cu: ≤0.50

Fabrication for Inconel 690 alloy:

INCONEL 690 alloy is readily fabricated by converntional techniques for high-nickel alloys. In most working operations, alloy 690 exhibits characteristics similar to those of INCONEL 600. Inconel 690 should be clean before it is heated and should be heated in a low sulfur atmosphere. Furnace atmospheres for open heating should also be slightly reducing to prevent excessive oxidation of the material.




Wednesday, 4 January 2017

Inconel 686 Alloy Properties, Fabrication & Corrosion

Inconel 686 Alloy Properties


Inconel 686 (UNS N06686)alloy is a low carbon, the most highly alloyed corrosion-resistant alloy, which is outstanding resistance to oxidizing, reducing, and mixed acid environments.

Fabrication for Inconel 686

Hot forming should be between 1600 and 2500℉(870 and 1230℃), with all heavy forming above 2000℉(1090℃). Work hardening during cold forming may make intermediate annealing necessary. Inconel 686 is normally annealed at 2150-2200℉(1180-1200℃), with rapid cooling.

Corrosion of Inconel 686 alloy

1. Resistance to General corrosion: 

General corrosion, an even, uniform attack of the alloy surface, is the most commonly encountered form of corrosion. This type of attack is predictable, which allows effective estimation of the life of components. The corrosion rate is significantly affected by the concentration of the corrosive medium, the presence of contaminants in the medium, and temperature.

15% HCI Boiling: 2mpy
80% H2SO4,93℃: 29mpy
90% H2SO4, 93℃: 8mpy
FGD1, 80℃: 23mpy
FGD2, 105℃: 274mpy

*mpy can be converted to mm/a by multiplying by 0.0254; FGD1: 60%H2SO4+2.5%HCI+0.2%HF+0.5% flyash at 80℃; FGD2: 70% H2SO4+2.5%HCI+0.2%HF at 105℃

2. Resistance to localized corrosion: 

Localized attack, pitting and crevice corrosion, can occur very quickly and lead to premature, unexpected failure. While the general attack of the surface of the component may be very light, a single pit may propagate throught the thickness of the part causing leakage and failure. Crevice corrosion, as the name implies, takes place within the crevices formed by overlapping sections of metal or under tightly adhering deposits.






Tuesday, 3 January 2017

Nickel 270 alloy/UNS N02270 Application and Physical Properties & Mechanical Properties

Nickel 270 Alloy Application



Nickel 270 alloy can applying at Hydrogen thyatron components, electrical resistance thermometers, platter bars, passive cathode, fluorescent lamp components, electrolytic cell anodes 

The Physical Properties of Alloy 270

Density: 8.91 g/cm3
Electrical Resistivity: 0.075μohm.m
Thermal Conductivity: 86 W/m.℃
Melting Range: 1454℃

The Mechanical Properties

Tensile Strength,min.:50ksi(345Mpa)
Yield Strength, min.: 16ksi(110Mpa)
Elongation: 50%
Hardness: 66max



  

Wednesday, 28 December 2016

Nickel 270 Properties Characteristic and Chemical Composition

Nickel 270/ UNS N02270/ ASTM F3 Properties Characteristic:


Nickel 270/ UNS N02270/ASTM F3/ W-Nr. 2.4050 is a high purity garde of nickel mad by power metallurgy, which has a low base hardness and high ductility. The extreme purity is useful for components of hydrogen thyratrons.

Chemical Composition of Nickel 270 Alloy

Nickel: ≥ 99.9
Copper: ≤0.01
Iron:  ≤0.05
Manganese: ≤0.003
Carbon: ≤0.02
Sulfur: ≤0.003
Titanium: ≤0.005
Magnesium: ≤0.005
Silicon: ≤0.005





Monday, 26 December 2016

Hastelloy G35 alloy Properties characteristic

Hastelloy G35 Alloy Properties characteristic

Hastelloy G35 Alloy Bar for Poland Client

Hastelloy G35 alloy is to provide corrosion resistance to the most difficult phosphoric acid enviroments. G35 alloy is much less susceptible to chloride-induced stress corrosion cracking than the stainless steels and nickel-chromium iron alloys traditionally used in"wet process" phosphoric acid. 

Due to its very high chromium content, G35 is extremely resistant to other oxidizing acids, such as nitric, and mixtures containing nitric acid. It possesses moderate resistance to reducing acids. Due to its appreciable molybdenum content, and unlike other nickel-chromium-molybdenum alloys, it's very resistant to "caustic de-alloying" in hot sodium hydroxide.




Thursday, 22 December 2016

Hastelloy G30 alloy Properties characteristic, Heat treatment & Fabrication

Hastelloy G30 alloy:


Hastelloy G30 alloy Seamless pipes 6meter

Properties characteristic:

Hastelloy G30 alloy is a high chromium nickel base alloy shows superior corrosion resistance over most other nickel and iron base alloys in commercial phosphoric acid and many complex environments containing highly oxidizing agents such as nitric acid.


Heat Treatment & Fabrication:

The annealing temperature for HASTELLOY G30 alloy is 1177℃(2150℉),and water quenching is advised(rapid air cooling is feasible with structures thinner than 10mm(0.375in). A hold time at the annealing temperature of 10 to 30 minutes is recommended, depending on the thickness of the structure(thicker structures need the full 30 minutes).

Hastelloy G30 alloy can be hot forged, hot rolled, hot upset, hot extruded, and hot formed. And it can apply in wire, sheet, plate, scrip, bar, Welded pipes& seamless pipes, forged.